| Material Technical Datasheet | ||||
| AC K03 | ||||
| Properties | Test Test | Mamiriro Emuedzo | Units | Tsika Dzakanaka |
| Proper Properties | ||||
| Specific Gravity | ASTM D792 | 23 ° C | g / cm³ | 1.22 |
| Shrinkage Rate Flow | ASTM D995 | 23 ° C | % | 0.8 |
| Shrinkage Rate Vertical | ASTM D995 | 23 ° C | % | 1.2 |
| Mvura Yekunyura Mwero 23°C 24hr | ASTM D570 | 23 ℃ | % | 0.2 |
| neukukutu | ||||
| Mechanical Properties | Test Test | Mamiriro Emuedzo | Units | Data |
| Rockwell kuoma R chiyero | ASTM D785 | 115 | ||
| Mechanical Properties | ||||
| Mechanical Properties | Test Test | Mamiriro Emuedzo | Units | Data |
| Kusimba Kusimba 23°C | ASTM D638 | 10mm / min | Mpa | 50 |
| Elongation 23°C | ASTM D638 | 10mm / min | % | 70 |
| Flexural Simba 23°C | ASTM D790 | 2.0mm / min | Mpa | 75 |
| Flexural Modulus 23°C | ASTM D790 | 2.0mm / min | Mpa | 2000 |
| Cantilever notch kukanganisa 23°C 3.2mm | ASTM D256 | 23 ° C A-notch | J / m | 600 |
| Cantilever isina notch impact -40°C | ASTM D256 | 23 ° C A-notch | J / m | 100 |
| Thermal Properties | ||||
| Thermal Properties | Test Test | Mamiriro Emuedzo | Units | Data |
| HDT | ASTM D648 | 0.45MPa | ℃ | 85 |
| HDT | ASTM D648 | 1.8MPa | ℃ | 60 |
| Kuita kweMagetsi | ||||
| Kuita kweMagetsi | Test Test | Data | Units | |
| Vhoriyamu kuramba | ASTM D257 | 1E17 | Cm.cm | |
| Surface kuramba | ASTM D257 | 1E15 | Ω | |
| Insulation simba 1.6mm | ASTM D149 | 30 | KV / mm | |
| Flame Retardancy | ||||
| Flame Retardancy | Test Test | Data | ||
| Moto Muyero Wakazara Ruvara 1.6mm | UL94 | HB | ||